Fix it in this order: a clean plate, the right bed temperature, then a slow first layer. Wipe the plate with isopropyl alcohol, or wash it with a few drops of washing-up liquid when that stops working, and keep your fingers off it. Set the bed to your filament maker’s range. Recalibrate only if the first layer still looks off.
Your first layer goes down, then a line drags behind the nozzle or the whole part slides off. On a printer that calibrates itself, such as the Bambu Lab A1 mini or the Flashforge Adventurer 5M with its one-click automatic levelling, a badly levelled bed is no longer the first suspect. Grease, temperature and first-layer settings are, so we leave levelling for last. If you haven’t printed anything yet, start with our guide to your first print.
Try this first: read the first layer
Watch the first layer go down and note what the lines do.
| What you see | Likely cause | Check first |
|---|---|---|
| Bare patches, or a part that slides off whole | Fingerprints or grease | Cause 1 |
| Lines go down, then lift behind the nozzle | Dirty plate or a bed that’s too cool | Causes 1 and 2 |
| Corners tear loose on fast moves | First layer too fast | Cause 3 |
| Round lines with gaps between them | Nozzle too far from the plate | Cause 5 |
| Lines squashed flat, with ridges between them | Nozzle too close to the plate | Cause 5 |
Then run the quick routine, in this order:
- Let the bed cool, then lift the plate off by its edges if it’s removable.
- Wipe the printing surface with 90% isopropyl alcohol; if the grip still fades, wash it in warm, not hot, water with a few drops of washing-up liquid.
- Dry it fully and refit it without touching the printing surface.
- Check the slicer’s bed temperature against the filament maker’s published range.
- Slow the first layer down and print again.
- Only if the lines show gaps or look squashed flat, rerun the printer’s calibration.
If the middle of the part stays down and only the corners curl up as it grows, that’s warping, not an adhesion fault: Prusa Research puts it down to plastic shrinking as it cools, mostly with high-temperature materials such as ABS and ASA. It has its own fixes, set out in how to stop corners lifting.
Why won’t the print stick? Causes, most likely first
Most often because something sits between the plastic and the plate. Let the printer cool before you lift the plate or touch the nozzle, and follow your manual before removing any part.
1. Grease and fingerprints on the plate
Symptom: patches where the lines won’t bond, or a print that slides off in one piece. Why: Flashforge says dust and grease build-up reduces adhesion. Prusa puts it simply: if you don’t touch the print surface with your hands or dirty tools, you don’t have to clean it.
Fix: for a quick wipe, Prusa recommends 90% isopropyl alcohol. When the grip fades even after that, wash the plate in warm water with a few drops of washing-up liquid and dry it well; Prusa says not to do this too often or submerge the sheet in hot water. Flashforge advises regular cleaning with water and a cleaning agent. From then on, hold the plate by its edges.
2. The bed is too cool for the filament
Symptom: the first lines go down, then lift as the nozzle passes, or let go a few layers in. Why: a generic slicer profile may not match your reel. Fix: set the bed to the range your filament maker publishes. If a new material still won’t stick, Prusa suggests raising the bed by 5–10 °C, within your printer’s limit: the A1 mini’s bed tops out at 80 °C.
| Filament | Bed, according to SUNLU | Nozzle, according to SUNLU |
|---|---|---|
| SUNLU PLA Filament | 50–60 °C | 200–210 °C at 50–100 mm/s |
| SUNLU PETG Filament | 60–70 °C | 240–260 °C |
| SUNLU TPU 95A Filament | 50–60 °C | 190–210 °C at 50–80 mm/s |
Makers differ: Prusa’s PETG guidance for its own printers asks for an 85 °C first-layer bed, above SUNLU’s range for the SUNLU PETG Filament and the A1 mini’s maximum. So start from your filament maker’s figures, not a generic number. Still choosing a plastic? Our PLA and PETG comparison sets out what each is good for.
If you don’t know what’s on your reel, start from a filament with published settings, such as the SUNLU PLA Filament in the table above.

Everyday 1.75 mm PLA on a 1 kg spool, with a ±0.02 mm diameter tolerance according to SUNLU, and bed and nozzle settings you can start from instead of guessing.
3. The first layer is too fast or too thin
Symptom: corners and short lines tear loose on quick changes of direction. Why: fast moves work against a first layer that hasn’t bonded yet; Prusa suggests about 75% of normal speed for the first three layers. Fix: lower the first-layer speed in your slicer and check the first-layer height. OrcaSlicer‘s documentation says a thicker first layer improves adhesion and makes up for small surface imperfections; it recommends 0.25 mm for a 0.4 mm nozzle, and no more than 65% of the nozzle diameter. If these settings are new to you, how a slicer works shows where to find them.
4. The plate surface doesn’t suit the filament
Symptom: PLA that won’t hold on a textured plate, or PETG that won’t let go of a smooth one. Why: smooth and textured PEI grip differently. Flashforge sells both for the Adventurer 5M series: its smooth PEI plate takes PLA, PETG and TPU with no glue, while its powder-coated, textured PEI plate may need glue. At the other extreme, Prusa warns that PETG can bond so hard to smooth PEI that it damages the sheet.
Fix: for PLA on a textured plate, work through causes 1 to 3 before you reach for glue. For PETG on smooth PEI, Prusa advises a glue stick as a separating layer, or a powder-coated sheet. If your slicer asks which plate is fitted, make sure it matches.
5. The nozzle is too high or too low
Symptom: Prusa’s calibration guide describes both. Too high: the lines aren’t flattened and leave gaps. Too low: the lines are squashed flat, with ridges between them; in the extreme, plastic so thin you can see through it, which can clog the hotend. Why: the gap has changed since the last calibration, for example after a nozzle swap or a move. Fix: rerun your printer’s calibration from its menu. On a printer you adjust by hand, Prusa’s advice is to judge the height by eye as the first layer prints, not by a set number.
Don’t lower the nozzle to make up for a dirty plate: Prusa warns against squashing the first layer to compensate for poor adhesion. And if gaps show on every layer, not just the first, read about thin, gappy walls instead.
6. The part has too little contact with the plate
Symptom: the first layer looks right, but a small or tall, narrow part gets knocked loose later. Fix: add a brim in your slicer; Prusa notes that it increases the surface area of the first layer. Keep glue stick as the last resort, once the plate, the temperature and the first layer are right. Prusa says a basic PVA glue stick is enough, and that in its experience PLA doesn’t need one.
When to recalibrate, and when to replace instead
Recalibrate after anything that changes the gap between nozzle and plate. Prusa’s list for its own printers is changing the nozzle, upgrading the extruder or moving the printer, and it keeps a separate first-layer setting for each print sheet because sheets differ in thickness. On a self-calibrating printer that’s a menu option, so there’s no reason to skip it.
Replace the plate when a clean plate, at the reel’s temperature and with a first layer that looks right, still won’t hold PLA anywhere: the surface may be worn. Buy the plate made for your model; Flashforge, for example, sells smooth PEI, textured PEI and PC plates for the Adventurer 5M series.
If your printer levels by hand and keeps drifting, a self-calibrating model removes that step. Our ranked list of 3D printers includes the A1 mini, our pick for a first printer, and you can compare every model on our 3D printer shelf.
Common questions
How often should I clean my 3D printer bed?
Whenever you’ve touched the printing surface or the grip starts to fade; Prusa says an untouched surface doesn’t need cleaning. Wipe it with isopropyl alcohol when it needs it, and save a wash for when that stops working.
Can I use washing-up liquid on a PEI plate?
Yes, unless your plate maker says otherwise. Prusa suggests a few drops in warm, not hot, water, without submerging the sheet, then drying it well. Flashforge recommends regular cleaning with water and a cleaning agent.
Do I need glue stick for PLA?
Usually not: Prusa says that in its experience PLA doesn’t need it, though Flashforge notes its textured PEI plate may need glue. Try a clean plate, the right bed temperature and a slower first layer first.
Why is PETG stuck so hard to my build plate?
On smooth PEI, PETG can bond so strongly that it damages the sheet, according to Prusa, which advises a glue stick as a separating layer or a powder-coated plate. Check your own plate maker’s advice too: Flashforge lists PETG for its smooth PEI plate without glue.
Sources
- First layer issues — Prusa Research
- First Layer Calibration (i3) — Prusa Research
- PETG — Prusa Research
- Warping — Prusa Research
- Build Plate for AD5M, AD5M Pro and AD5X — Flashforge